指标/产品 | 单位 | 常德镁砖 | 镁铝砖 | 镁锆砖 | 镁铬砖 | |||||
---|---|---|---|---|---|---|---|---|---|---|
WDMZ-98 | WDMZ-95 | WDMZ-97 | WMZ-80A | WMZ-80B | WMZ-1 | WMZ-2 | WDMC-12 | WDMC-20 | ||
MgO≥ | % | 97.5 | 95 | 97 | 80 | 80 | 73 | 77 | 60 | 58 |
CaO≤ | % | 1.2 | 2.0 | - | - | - | - | - | - | - |
Al2O3 ≥ | % | - | - | 5-10 | 5-10 | - | - | - | - | - |
SiO2≤ | % | 1.0 | 2.0 | - | - | - | - | - | 3.2 | 1.5 |
ZrO2≥ | % | - | - | - | - | 12 | 12 | 12 | ||
Cr2O3≥ | % | - | - | - | - | - | - | - | 12 | 20 |
显气孔率≤ | % | 16 | 18 | 18 | 18 | 20 | 18 | 16 | 19 | 18 |
常温耐压强度≥ | Mpa | 60 | 60 | 40 | 40 | 30 | 65 | 70 | 35 | 40 |
0.2Mpa荷重软化开始温度≥ | ℃ | 1700 | 1600 | 1600 | 1600 | 1580 | 1600 | 1600 | 1580 | 1650 |
重烧线变化1650℃x2h | % | - | - | - | - | - | - | - | - | |
体积密度≥ | g/cm³ | 3.05 | 2.9 | - | - | - | 3.0 | 3.1 | 3.0 | 3.0 |